Minigold is a gold-reduced casting alloy. Its composition makes it suitable for a wide range of indications and its golden yellow colour allows natural shade effects in the restoration veneered with laboratory composite SR Nexco.
Composition (%): | Au 40.0 | Pd 4.0 | Ag 47.0 | Cu 7.5 | Zn 1.0 | In <1.0, Ir <1.0 |
ISO | 22674:2016 |
ADA Type | Noble |
Type / Colour | 4 / Yellow |
Density (g/cm³) | 12.4 |
Melting Range (Solidus/Liquidus): | 865 - 945 °C |
Elastic Modulus (GPa): | 88 |
As Cast Softened Hardened | |
Vickers Hardness: | 190 125 215 |
Tensile Strength (MPa): | 600 400 680 |
0.2% Proof Stress (MPa): | 430 280 540 |
Elongation (%): | 15 30 12 |
Investment Material: | Phosphate-bonded / Gypsum-bonded |
Preheating / Burn- out Temperature: | 650 - 760 °C |
Crucible | Carbon crucible / Ceramic crucible |
Casting Temperature: | 1000 - 1050 °C |
Recommended Lab Composite: | SR Nexco |
Laser Welding Wire: | Laser C&B Yellow |
*See TYPE CLASSIFICATION DUE TO PHYSICAL PROPERTIES